Characterization of Bi2O3 nanoparticles

Figure 1a presents the TEM micrograph of Bi2O3 nanoparticles, revealing the formation of a dark, spherical, and uniformly distributed morphology with an average diameter ranging from 2 to 21 nm. Additionally, the TEM image indicates that most particles are well dispersed with limited agglomeration, which can be attributed to the high surface energy and nanoscale nature of the particles. The homogeneous distribution and small particle size are advantageous for enhancing the interfacial interaction between Bi2O3 nanoparticles and the polymer matrix in nanocomposite applications.

The XRD pattern of Bi2O3 nanoparticles (Fig. 1b) reveals a well-crystallized monoclinic α-phase structure, consistent with JCPDS card No. 41-1449. The diffractogram exhibits a series of distinct and sharp diffraction peaks, confirming the high crystallinity of the synthesized nanoparticles. The two most intense peaks appear at 2θ = 27.44° and 28.06°, corresponding to the (002) and (200) crystallographic planes, respectively, which are the characteristic signature reflections of the monoclinic Bi2O3 phase.37,38. Additional peaks are observed at 2θ = 23.97° (120), 25.91° (021), 31.77° (121), 32.69° (220), 33.30° (012), 35.07° (211), 36.26° (022), 39.46° (122), 41.13° (300), 46.34° (222), 47.21° (040), 52.45° (141), 55.79° (004), 57.83° (321), and 64.12° (421). The sharp and intense diffraction peaks confirm the crystalline nature and high purity of the synthesized Bi2O3 nanoparticles.

Fig. 1Fig. 1

(a) TEM micrograph and (b) XRD pattern of Bi2O3 nanoparticles.

Mechanical properties of LDPE/PVB blend

Figure 2 illustrates the effect of PVB ratio (3, 5, and 10%) on the mechanical properties of LDPE/PVB blends, including tensile strength, elongation at break, and elastic modulus. It is known that the mechanical properties of a blend of two polymers depend mainly on the compatibility between the two polymers, blend ratio, and any compatibilizers used during processing. It is known that LDPE is flexible, ductile, chemically resistant, and has good elongation at break, but relatively low strength and stiffness. On the other hand, PVB is flexible, adhesive, tough, and has excellent impact resistance.

The tensile strength (Fig. 2a) increased from 13.3 MPa for neat LDPE to 14.8 MPa and 15.5 MPa for blends containing 3 and 5 wt% PVB, respectively. This improvement indicates enhanced stress transfer and favorable interfacial interactions between LDPE and the dispersed PVB phase. However, when the PVB content was increased to 10 wt%, the tensile strength decreased to about 13.9 MPa, suggesting that excessive PVB loading may lead to phase separation or the formation of stress concentration sites, which negatively affect the mechanical performance of the blend. The elongation at break (Fig. 2b) showed a continuous decrease with increasing PVB content. Neat LDPE exhibited a high elongation at break of 860%, reflecting its highly ductile nature. The elongation decreased to about 780%, 620%, and 600% for blends containing 3, 5, and 10 wt% PVB, respectively. This reduction indicates that the incorporation of PVB into LDPE texture enhances the stiffness of the polymeric matrix and hence decreases the elongation percent39. A similar trend was observed for the elastic modulus (Fig. 2c) as in tensile strength. The elastic modulus increased from 9.6 MPa for neat LDPE to 10.4 MPa and reached a maximum value of 10.8 MPa at 5 wt% PVB, demonstrating an increase in stiffness due to the reinforcing effect of PVB. However, further increasing the PVB content to 10 wt% caused a significant decrease in elastic modulus to 6.7 MPa, which may be attributed to reduced blend homogeneity and weaker interfacial interaction at higher PVB concentrations. Based on the results, the incorporation of 5 wt% PVB provides the optimum balance between strength and stiffness while maintaining reasonable ductility. The enhancement in tensile strength and elastic modulus at low PVB contents confirms the effectiveness of PVB as a reinforcing component in LDPE. The results indicated that the optimum LDPE/PVB blend ratio was 95/5 wt%.

Fig. 2Fig. 2

Mechanical properties of LDPE/PVB blends containing different PVB contents; (a) tensile strength, (b) elongation at break (%), and (c) elastic modulus.

Effect of EB irradiation on the mechanical properties of LDPE/PVB/Bi2O3 nanocomposites

Figure 3 presents the effect of electron-beam irradiation dose on the mechanical properties (tensile strength, elongation at break, and elastic modulus) of LDPE/5%PVB loaded with a fixed ratio of 3 phr Bi2O3 nanocomposites. LDPE is a nonpolar polymer, whereas PVB contains polar hydroxyl groups; consequently, LDPE/PVB blends are generally characterized by limited compatibility and partial immiscibility. The poor interfacial interaction between the two polymer phases can adversely affect the mechanical properties of the blend. Therefore, EB irradiation was employed at doses of 10, 30, 50, 100, 120, and 150 kGy to enhance interfacial interactions and improve the compatibilization between the LDPE and PVB matrices through radiation-induced crosslinking. As shown in Fig. 3a, the tensile strength of LDPE/PVB/Bi2O3 nanocomposites increased progressively with rising EB irradiation dose. It rose from 13.3 MPa for the unirradiated sample to 14.3, 14.7, and 15.4 MPa at 10, 30, and 50 kGy, respectively. A pronounced enhancement was observed at higher doses (100–120 kGy), reaching 17.0 MPa, whereas at 150 kGy a slight decrease was predominant.

This enhancement is attributed to radiation-induced crosslinking within the polymer matrix, which strengthens the interfacial interactions among LDPE, PVB, and Bi₂O₃ nanoparticles. The elongation at break (Fig. 3b) also exhibited a remarkable increase with rising irradiation dose, reaching its maximum at 100 kGy. The observed increase in elongation in the presence of Bi₂O₃ may be linked to the strain-induced crystallization effect commonly reported in polymer composites39,40. At higher doses (120–150 kGy), however, the elongation declined, reflecting the increased stiffness and restricted chain mobility within the polymer matrix.

The elastic modulus (Fig. 3c) of LDPE/PVB/Bi2O3 nanocomposites increased steadily with rising electron-beam irradiation dose. It rose from 9.6 MPa for the unirradiated sample to 10.0, 10.6, and 10.8 MPa at 10, 30, and 50 kGy, respectively. A further enhancement was observed at higher doses, reaching 11.3 MPa at 100 kGy, followed by slight increments at 120–150 kGy, indicating a gradual approach toward saturation in stiffness improvement. EB irradiation effectively enhanced the mechanical properties of the LDPE/PVB/Bi2O3 nanocomposite by improving crosslinking and interfacial compatibility within the polymer matrix. Among the studied doses, 100 kGy yielded the best overall mechanical performance, indicating the most favorable balance between network formation and structural stability. The results are consistent with previous reports on LDPE/carbon black nanocomposites; moreover, EB irradiation at 100 kGy was shown to yield optimal mechanical performance and increased crosslinking, supporting the interpretation that irradiation effectively modifies the polymer network and surface morphology.41

Fig. 3Fig. 3

Effect of irradiation dose on the mechanical properties of LDPE/PVB/Bi2O3 nanocomposite: (a) tensile strength, (b) elongation at break, and (c) elastic modulus.

Effect of EB-irradiation on gel fraction and crosslink density

The effect of irradiation dose on the gel fraction of the LDPE/PVB/Bi2O3 nanocomposite is shown in Fig. 4a. The gel fraction increases markedly with increasing irradiation dose from 10 to 100 kGy, followed by a nearly constant value at higher doses (120–150 kGy). The unirradiated sample exhibits a very low gel fraction of about 5%. As the irradiation dose increases to 10, 30, 50, and 100 kGy, the gel fraction increases to approximately 17, 38, 67, and 92%, respectively. Above 100 kGy, only a slight increase is observed, reaching 93–94% at 125–150 kGy. The initial increase in gel fraction is attributed to radiation-induced generation of macroradicals along the LDPE/PVB polymer chains. These subsequently recombine to form intermolecular crosslinks and progressively develop a three-dimensional polymer network. The presence of the polar PVB may also contribute to the development of the network because irradiation can generate reactive sites in the polymer blend, facilitating intermolecular reactions between the constituent chains. Similar dose-dependent increases in gel fraction have been reported for irradiated polyethylene, where increasing irradiation dose promotes the formation of a crosslinked network42.

The crosslink density of the LDPE/PVB/Bi2O3 nanocomposite increased with increasing EB irradiation dose, indicating progressive formation of a three-dimensional crosslinked network within the polymer matrix as shown in Fig. 4b. The enhanced crosslink density restricts molecular-chain mobility and improves the structural integrity of the composite. At higher irradiation doses, the crosslink density tends to approach a plateau, suggesting that most available reactive sites have been consumed and further irradiation produces only a limited increase in network formation. Overall, the results confirm that irradiation effectively promotes crosslinking of the LDPE/PVB/Bi2O3 nanocomposite at 100 kGy, providing a highly developed crosslinked structure, which is considered an optimum dose for achieving a highly crosslinked LDPE/PVB/Bi2O3 nanocomposite. Studies on irradiated LDPE have shown that increasing radiation dose increases crosslink density.43 Additionally, the results are consistent with previous reports that EB irradiation increased crosslink density and improved interfacial interaction after irradiation.44

Figure 5 presents the schematic mechanism of interaction among LDPE, PVB, and Bi2O3 nanoparticles under EB irradiation. Irradiation induces bond scission in both LDPE and PVB chains, generating reactive polymer radicals. These radicals follow three principal pathways: LDPE–LDPE crosslinking via radical recombination, LDPE–PVB coupling that enhances polymer–polymer compatibility, and interfacial bonding between PVB hydroxyl groups and Bi2O3 nanoparticles through hydrogen bonding/coordination. Collectively, these processes yield a dense, integrated polymeric network reinforced by Bi2O3 nanoparticles, which improves structural properties and enhances the physicochemical performance of the LDPE/PVB/Bi2O3 nanocomposite.

Fig. 4Fig. 4

Effect of EB irradiation dose on the gel fraction (%) and crosslinking density of LDPE/PVB/Bi2O3 nanocomposites.

Fig. 5Fig. 5

Schematic mechanism of interaction of LDPE, PVB, and Bi2O3 nanoparticles during EB irradiation.

FTIR results

Figure 6 presents the FTIR spectra of LDPE, PVB, LDPE/PVB (95/5) blend, and irradiated LDPE/PVB/Bi2O3 nanocomposite. The FTIR spectrum of neat LDPE (Fig. 6a) exhibits the characteristic absorption bands of polyethylene. The strong peaks observed at 2916 and 2848 cm− 1 correspond to the asymmetric and symmetric stretching vibrations of –CH₂ groups, respectively. The bands at around 1463 cm− 1 and 720 cm− 1 are attributed to CH₂ bending (scissoring) and rocking vibrations of long-chain methylene groups, confirming the typical molecular structure of LDPE45. The spectrum of PVB (Fig. 6b) displays several characteristic absorption bands associated with its functional groups. A broad absorption band centered around 3440 cm− 1 is assigned to the stretching vibration of hydroxyl (–OH) groups. The peaks near 2930–2870 cm− 1 correspond to aliphatic C–H stretching vibrations. The absorption band observed around 1724 cm− 1 is attributed to the carbonyl (C = O) stretching of residual vinyl acetate groups. The absorption band near 1450 cm− 1 is assigned to C–H bending vibrations of methylene and methyl groups, while bands in the range of 1100–1000 cm− 1 are associated with C–O–C and C–O stretching vibrations of the butyral structure. These characteristic absorption bands collectively confirm the presence of butyral acetal, hydroxyl, and acetate functionalities of PVB46,47,48. In the FTIR spectrum of the LDPE/PVB (95/5) blend (Fig. 6c), the incorporation of PVB introduces several additional absorption bands associated with its functional groups. In addition, the spectrum contains the principal absorption bands of both LDPE and PVB, indicating successful blending between them. Slight broadening and minor shifts in some absorption bands suggest intermolecular interactions between the hydroxyl groups of PVB and the polyethylene matrix. The characteristic CH₂ stretching bands of LDPE appeared at 2916 and 2848 cm− 1, while the broad hydroxyl band of PVB appeared with reduced intensity due to its lower concentration in the blend. The presence of both polymer-specific bands. In addition, the band observed near 1463 cm−1is assigned to CH₂ bending (scissoring) vibrations, while the characteristic CH₂ rocking vibration appearing around 723 cm− 1 serves as a fingerprint band for polyethylene crystallinity. The characteristic PVB peaks appearing at 1132 cm− 1 and 995 cm− 1 correspond to the C–O–C stretching vibration of the butyral ring and C–O stretching vibrations, respectively, confirming the presence of acetal functionalities in the blend. Furthermore, the absorption band observed near 1698 cm− 1 is assigned to the C = O stretching vibration of residual vinyl acetate groups. Another band detected around 1377 cm− 1 represents a characteristic polyolefin-related vibration associated with LDPE19. The FTIR spectrum of the LDPE/PVB/ Bi2O3 nanocomposite (Fig. 6d) retains the characteristic absorption bands of the LDPE/PVB blend, indicating that the fundamental chemical structures of both polymers remain unchanged after incorporation of Bi2O3 nanoparticles. The FTIR spectrum of PVB exhibits characteristic absorption bands at 1132 and 995 cm⁻¹, corresponding to C–O stretching vibrations. Upon incorporation of Bi2O3 nanoparticles, slight changes in band intensity and small shifts are observed in the hydroxyl and C–O stretching regions. These spectral modifications reflect specific interactions between Bi2O3 and the functional groups of PVB, indicating successful integration of the nanoparticles within the polymer matrix. Furthermore, the appearance or enhancement of weak absorption bands in the 500–650 cm− 1 region can be attributed to Bi–O stretching vibrations, confirming the successful incorporation of Bi2O3 nanoparticles within the polymer matrix49. The absence of new major absorption bands indicates that the nanoparticles are physically dispersed within the blend rather than chemically altering the polymer backbone. Additionally, EB irradiation can improve interfacial interaction between components, enhance nanoparticle dispersion, and increase crosslink density, leading to improved mechanical, thermal, and surface properties.

Fig. 6Fig. 6

FTIR spectrum of (a) LDPE, (b) PVB, (c) LDPE/PVB blend (95/5), and (d) LDPE/PVB/Bi2O3 nanocomposite.

XRD results

Figure 7 represents the XRD patterns of LDPE, PVB, LDPE/PVB blend, LDPE/PVB/Bi2O3, and irradiated LDPE/PVB/Bi2O3 nanocomposite at 100 kGy, which provide important information about the crystalline structure and phase distribution of the prepared materials. The patterns clearly demonstrate the coexistence of the crystalline LDPE phase, the predominantly amorphous PVB phase, and the crystalline Bi2O3 phase, together with structural modifications induced by electron-beam irradiation.

Neat LDPE (Fig. 7a) exhibits two intense and well-defined diffraction peaks at 2θ = 21.4° and 23.7°, which are assigned to the (110) and (200) planes, respectively, of the crystalline structure of LDPE. The pronounced intensity of these reflections confirms the semicrystalline nature of LDPE50,51,52. In contrast, the XRD pattern of PVB (Fig. 7b) shows a broad diffraction halo centered around 2θ ≈ 19.2°. This broad feature is characteristic of the predominantly amorphous structure of PVB53,54. Upon blending PVB with LDPE, the LDPE characteristic (110) and (200) reflections remain visible in the XRD pattern of the LDPE/PVB blend (Fig. 7c), indicating that incorporation of PVB does not destroy the basic crystalline structure of LDPE. However, the relative intensity and broadness of the diffraction profile are modified because of the contribution of the amorphous PVB phase and interactions between the two polymer components. This suggests that the LDPE crystalline domains are retained within the polymer blend with good compatibility between LDPE and PVB.

Upon incorporation of Bi2O3, the LDPE/PVB/Bi2O3 nanocomposite (Fig. 7d) retained the characteristic crystalline peaks of LDPE, while exhibiting slight peak broadening and reduced diffraction intensity. In addition, weak diffraction features corresponding to Bi2O3 nanoparticles appeared, confirming their successful incorporation into the polymer matrix. These changes can be attributed to the homogeneous nanoscale dispersion of Bi2O3 nanoparticles and are consistent with enhanced interfacial compatibility with the LDPE/PVB polymer chains, which slightly modified the crystalline arrangement of the composite system.

For the LDPE/PVB/Bi2O3 nanocomposite (Fig. 7d), the characteristic LDPE reflections remain evident, while additional weaker reflections appear at higher diffraction angles and are assigned to the crystalline Bi₂O₃ phase, including the indexed reflections shown in the figure, such as (002), (200), (211), and (122). The simultaneous presence of the LDPE and Bi₂O₃ reflections confirms the successful incorporation of the inorganic oxide into the polymer matrix. The absence of a substantial amorphous background increase or disappearance of the principal LDPE peaks indicates that Bi2O3 incorporation does not completely disrupt the semicrystalline structure of LDPE. After EB irradiation of the LDPE/PVB/Bi2O3 nanocomposite at 100 kGy (Fig. 6e), the main LDPE reflections are still observed, demonstrating that the fundamental crystalline structure of the LDPE matrix is preserved after irradiation. At the same time, several additional Bi₂O₃-related reflections become more distinguishable, including the indexed (002), (200), (220), (121), (122), (222), (141), and (004) reflections. The persistence of these characteristic oxide reflections confirms the structural stability of the Bi2O3 nanoparticles during electron-beam processing. Therefore, the XRD results support the formation of an LDPE/PVB/Bi₂O₃ nanocomposite in which the LDPE crystalline phase and Bi₂O₃ crystalline phase are maintained, while electron-beam irradiation primarily modifies the polymer network through radiation-induced crosslinking rather than producing a new crystalline phase, supporting the formation of a stable crosslinked LDPE/PVB/Bi2O3 nanocomposite.

Fig. 7Fig. 7

XRD curves of (a) LDPE, (b) PVB, (c) LDPE/PVB blend, (d) unirradiated LDPE/PVB/Bi2O3, (e) LDPE/PVB/Bi2O3 nanocomposite irradiated at 100 kGy.

Surface morphology

The SEM micrographs in Fig. 8 show the morphological evolution of LDPE after incorporation of PVB, Bi2O3 nanoparticles, and subsequent electron-beam irradiation at 100 kGy. The SEM micrograph of neat LDPE (Fig. 8a) reveals a relatively smooth, compact, and homogeneous surface. The absence of pronounced cracks, voids, or phase-separated domains highlights the uniform morphology, good structural integrity, and stable polymeric nature of the LDPE matrix. This smooth appearance further reflects its ductile character and excellent film-forming capability.

Figure 8b shows the SEM of LDPE/PVB after incorporation of 5 wt% PVB into LDPE; the surface becomes rougher and more fibrillar in morphology, with elongated streaks and irregular surface features. Nevertheless, no large cavities or severe phase separation are apparent, indicating reasonably good compatibility between LDPE and PVB.

Upon incorporation of Bi2O3 nanoparticles into the LDPE/PVB blend (Fig. 8c), the nanocomposite surface exhibits a more regulated morphology with uniformly distributed, highly dispersed nanoparticles. The absence of extensive agglomeration indicates effective nanoparticle dispersion within the polymer matrix, contributing to improved structural uniformity. Similar morphological characterization of LDPE/Bi2O3 nanocomposites by SEM has demonstrated the influence of Bi2O3 incorporation on the surface morphology and filler dispersion within the polyethylene matrix.55.

After irradiation, the SEM of LDPE/PVB/Bi2O3 at 100 kGy (Fig. 8d) shows that the nanocomposite exhibits a more compact and relatively homogeneous morphology, with a reduction in pronounced grooves and surface defects compared with the non-irradiated nanocomposite. The smoother morphology can be attributed to EB-induced crosslinking, which promotes intermolecular bonding and network formation within the polymer matrix. The resulting crosslinked structure can restrict polymer-chain mobility, improve interfacial interactions among LDPE, PVB, and Bi2O3, and reduce the development of voids or interfacial defects. The improved morphological integrity is therefore consistent with the enhanced mechanical and radiation-resistant properties of the irradiated nanocomposite. The results are consistent with LDPE/Bi2O3 nanocomposites, as confirmed by SEM analysis, which effectively demonstrates Bi2O3 nanoparticle dispersion and the resulting surface morphology.55.

Fig. 8Fig. 8

SEM micrographs of (a) neat LDPE, (b) LDPE/PVB (95/5) blend, (c) LDPE/PVB/Bi2O3 nanocomposite, and (d) irradiated LDPE/PVB/Bi2O3 nanoconposite at 100 kGy.

Thermal stability

Figure 9 represents the TGA curves of LDPE, LDPE/PVB, LDPE/PVB/Bi2O3, and irradiated LDPE/PVB/Bi2O3 nanocomposite at 100 kGy, demonstrating the influence of PVB blending, Bi2O3 nanoparticles, and EB irradiation on the thermal stability of LDPE-based composites. The TGA curves reveal the thermal degradation behavior of four material systems over a temperature range of 30 °C to 600 °C. All samples remain thermally stable up to around 200–250 °C, showing negligible mass loss during this initial stage. The neat LDPE sample exhibits the lowest thermal stability, showing an earlier onset of degradation and rapid weight loss within the temperature range of 330–470 °C due to the thermal decomposition of polyethylene chains, leaving a residual mass of 2–3%. After blending with PVB, the LDPE/PVB composite displays improved thermal resistance, as evidenced by the shift of the degradation curve toward higher temperatures and the slower decomposition rate. This enhancement suggests that the incorporation of PVB provides a modest improvement in thermal stability compared with pure LDPE, attributed to the improved intermolecular interactions within the LDPE/PVB polymer matrix.

The incorporation of Bi2O3 nanoparticles into the LDPE/PVB matrix further enhances the thermal stability of the composite. The LDPE/PVB/Bi2O3 sample shows a delayed degradation process and weight loss within the temperature range of 430 °C and higher, with residual mass at elevated temperatures, indicating that Bi2O3 nanoparticles act as thermal barriers that restrict the mobility of polymer chains and retard the diffusion of volatile decomposition products. Moreover, the nanoparticles may promote char formation and improve heat dissipation during thermal decomposition. The irradiated LDPE/PVB/Bi2O3 nanocomposite at 100 kGy exhibits the highest thermal stability among all investigated samples. The TGA curve shifts noticeably toward higher temperatures, with a slower and more gradual weight loss process. This behavior suggests that irradiation at 100 kGy induces crosslinking within the polymer matrix, enhancing intermolecular bonding and reducing chain scission. In addition, the synergistic effect of irradiation and Bi2O3 nanoparticles contributes to the formation of a more compact and thermally resistant network structure. Consequently, the irradiated nanocomposite retains a higher percentage of its mass at elevated temperatures, confirming its superior thermal durability and resistance to thermal degradation.

Fig. 9Fig. 9

TGA curves of neat LDPE, LDPE/PVB blend, LDPE/PVB/Bi2O3 unirradiated, and irradiated LDPE/PVB/Bi2O3 nanocomposite irradiated at 100 kGy.

Contact angle measurement

The surface hydrophobicity of materials can be quantitatively evaluated by measuring the water contact angle, which provides a direct indication of surface wettability. A lower contact angle corresponds to greater water spreading and, consequently, higher surface wettability and lower hydrophobicity, whereas a higher contact angle indicates reduced wettability, enhanced hydrophobicity, and greater water repellency. A contact angle less than 90° indicates a hydrophilic surface, meaning the surface has a high affinity for water and allows the droplet to spread more readily. In contrast, a contact angle greater than 90° indicates a hydrophobic surface, reflecting a lower affinity for water and a more spherical droplet shape. Therefore, an increase in contact angle corresponds to an increase in the hydrophobicity of the surface, while a decrease in contact angle indicates greater surface wettability.

The contact angle measurements presented in Fig. 10 clearly demonstrate the effects of PVB incorporation, Bi2O3 nanoparticle addition, and EB irradiation on the surface wettability and hydrophobicity of the LDPE-based composites. The neat LDPE film exhibits a contact angle of 93°56, indicating its intrinsically hydrophobic nature, which can be attributed to its nonpolar hydrocarbon backbone and relatively low surface energy. As observed in the inset photograph, the water droplet retains a relatively hemispherical shape with limited spreading across the LDPE surface, confirming its moderate water repellency and low surface wettability.

Following blending of LDPE with PVB, the contact angle of LDPE/PVB increases to 112°, indicating a clear enhancement in surface hydrophobicity compared with the pristine LDPE film. This increase may be attributed to the alteration of surface morphology and intermolecular interactions arising from the incorporation of PVB, which can modify the surface roughness and chemical characteristics of the blend.

The incorporation of Bi2O3 nanoparticles into the LDPE/PVB matrix at 0 kGy increases the water contact angle to 124°, indicating a pronounced enhancement in surface hydrophobicity. This improvement can be attributed to the presence of Bi2O3 nanoparticles enhance the surface stability of the composite and contribute to reduced surface wettability. This result is consistent with previous studies reporting that the incorporation of nanoparticles into polymeric composite films can increase surface roughness and hydrophobicity, thereby leading to an increase in the water contact angle.57

After EB irradiation at 100 kGy, the LDPE/PVB/Bi2O3 nanocomposite exhibits the highest water contact angle of 142°, indicating a pronounced enhancement in surface hydrophobicity and water-repellent behavior, which consequently suggests improved self-cleaning potential. This behavior can be attributed to the synergistic effect between Bi2O3 nanoparticles and EB irradiation, while promote the formation of hierarchical surface features, further reducing water-surface interactions and enhancing water repellency. Overall, the contact angle results confirm that the incorporation of PVB and Bi2O3 nanoparticles, combined with EB irradiation, significantly improves the hydrophobicity and potential self-cleaning properties of the LDPE-based nanocomposites.

The inset photographs show a small water droplet deposited on the surfaces of the LDPE-based samples to evaluate their surface wettability, with the contact angle determined at the three-phase contact line between the droplet and the solid surface. The droplets exhibit increasingly rounded, dome-like shapes with increasing contact angle, indicating progressively reduced water spreading and enhanced hydrophobicity. The contact angle increased from 95° for LDPE to 108° for LDPE/PVB and 121° for the unirradiated LDPE/PVB/Bi2O3 nanocomposite, while irradiation at 100 kGy further increased the contact angle to 139°, producing the most pronounced droplet curvature and the lowest surface wettability. These photographic observations are in good agreement with the measured contact-angle values, confirming the progressive enhancement of the water-repellent character of the nanocomposite surface.

Fig. 10Fig. 10

Contact angle measurements of LDPE film, LDPE/PVB, the unirradiated LDPE/PVB/Bi2O3, and the irradiated LDPE/PVB/Bi2O3 at 100 kGy.

Self-cleaning performance

Figure 11 depicts the self-cleaning performance of LDPE, LDPE/PVB, LDPE/PVB/Bi2O3, and irradiated LDPE/PVB/Bi2O3 nanocomposite, evaluated through the photodegradation of MB dye under UV irradiation. As shown in Fig. 11A, the degradation efficiency of pristine LDPE reaches only 16% after 8 h of UV irradiation, whereas LDPE/PVB achieves 48%. Incorporation of Bi2O3 nanoparticles markedly enhances the efficiency to 83%, underscoring their effective photocatalytic role in generating reactive oxygen species that decompose organic dye molecules. Notably, the irradiated LDPE/PVB/Bi2O3 nanocomposite exhibits the highest performance, approaching 94% degradation after 8 h of irradiation. The enhanced photocatalytic self-cleaning performance of the irradiated nanocomposite arises from multiple synergistic factors. First, Bi2O3 nanoparticles serve as active photocatalytic centers, absorbing UV light and generating electron–hole pairs that subsequently yield highly reactive radicals responsible for dye degradation. Second, irradiation treatment improves nanoparticle dispersion and strengthens interfacial interaction within the polymer matrix, thereby increasing the density of accessible active sites, facilitating charge separation, and suppressing electron–hole recombination. Consequently, the irradiated LDPE/PVB/Bi2O3 nanocomposite exhibits markedly superior photocatalytic efficiency and self-cleaning capability. Figure 11B presents photographic images showing the progressive discoloration of MB dye on the sample surfaces as a function of UV irradiation time. Upon UV exposure, the intensity of the blue coloration gradually decreases; however, the rate of dye removal strongly depends on the composition of the tested material. Pristine LDPE exhibits the lowest self-cleaning activity, retaining a considerable fraction of the dye even after 8 h of irradiation. Incorporation of PVB slightly improves stain degradation, producing a more noticeable reduction in color intensity compared with neat LDPE. A substantial enhancement is achieved with the addition of Bi2O3 nanoparticles, where the stain fades rapidly and becomes nearly invisible after extended irradiation. The irradiated LDPE/PVB/ Bi2O3 nanocomposite demonstrates the most pronounced self-cleaning behavior, with near-complete disappearance of the MB stain after only 4 h of UV exposure, confirming its superior photocatalytic activity. This improvement was attributed to the enhanced generation of reactive species, improved nanoparticle dispersion, and irradiation-induced surface modifications.

The photocatalytic efficiency obtained for the irradiated LDPE/PVB/Bi2O3 nanocomposite (94% MB degradation after 8 h of UV irradiation) is superior to many reported polymer-supported photocatalysts. For example, cellulose acetate membranes containing ZnO nanoparticles58 degraded only about 30% of MB under UV irradiation and approximately 75% under simulated sunlight, indicating lower photocatalytic activity than that achieved in the present work. In addition, Bi2O3-containing photocatalysts have demonstrated excellent dye degradation capability, with Bi2O3–Al2O3 nanocomposites59 achieving nearly 90% MB degradation under optimized UV irradiation conditions. These comparisons suggest that the synergistic combination of Bi2O3 nanoparticles and EB irradiation in the present study provides a highly efficient strategy for developing multifunctional self-cleaning polymeric materials.

Table (1) presents a comparison of different polymer-supported photocatalytic systems for MB degradation, revealing that performance is strongly influenced by both material composition and processing method. Cellulose acetate/ZnO membranes exhibited only modest activity (~ 30% MB removal under UV), underscoring the limited efficiency of simple ZnO incorporation. In contrast, Bi2O3–Al2O3 nanocomposites achieved ~ 90% degradation under optimized UV conditions, highlighting the superior photocatalytic potential of bismuth oxide systems. PVC films embedded with Bi-based heterostructures have also been reported to provide self-cleaning and antibacterial properties, confirming the versatility of Bi-based photocatalysts in polymer matrices. Beyond these polymer supports, Bi-based powders and thin films (e.g., BiVO4, Bi2WO6, BiOX) have demonstrated high visible-light activity, while biorenewable nanocomposites offer sustainable adsorption–photocatalysis synergy for immaculate water production. Building on these findings, the present work introduces LDPE/PVB/Bi2O3 nanocomposites fabricated by EB irradiation, which not only improved mechanical, thermal, and wettability properties but also achieved 94% MB degradation after 8 h UV exposure. This demonstrates that radiation processing can significantly enhance photocatalytic efficiency while simultaneously tailoring multifunctional properties, positioning the developed system as a promising candidate for advanced wastewater treatment applications (Table 1).

Fig. 11Fig. 11

Self-cleaning performance of (a) LDPE, (b) LDPE/PVB, (c) unirradiated LDPE/PVB/Bi2O3, and (d) irradiated LDPE/PVB/Bi2O3 at 100 kGy, evaluated by the photocatalytic degradation of MB dye under UV irradiation. (A) Degradation efficiency (%) as a function of irradiation time, and (B) photographic images illustrating the progressive discoloration of MB stains on the sample surfaces during UV exposure.

Table 1 Comparison of photocatalytic systems for MB degradation.Photocatalytic kinetics

The kinetics of photocatalytic degradation of MB were analysed using pseudo-first-order and pseudo-second-order models as expressed in Eqs. 4–5.

$$\:\text{ln}\left({C}_{0}-{C}_{t}\right)=\:{K}_{1}t$$

(4)

$$\:\frac{t}{{C}_{t}}=\:\frac{1}{{k}_{2}{{C}_{0}}^{2}}+\:\frac{t}{{C}_{0}}$$

(5)

where C0 is the initial MB concentration, Ct is the MB concentration at time t, and k1 is the pseudo-first-order rate constant, and k2 is the pseudo-second-order rate constant.

Table 2 shows that the pseudo-first-order kinetic model provides excellent linear fits, with correlation coefficients (R2) ranging from 0.985 to 0.998, indicating that the degradation of MB is predominantly governed by photocatalytic reaction kinetics. The apparent rate constant (k1) increased systematically from 0.073 h⁻¹ for neat LDPE to 0.351 h⁻¹ for the LDPE/PVB/Bi2O3 nanocomposite irradiated at 100 kGy, demonstrating that the incorporation of Bi₂O₃ and EB irradiation significantly enhances the MB degradation rate.

The pseudo-second-order model also showed good agreement with the experimental data, with R2 values ranging from 0.981 to 0.996, indicating that adsorption and surface interactions also contribute to the overall MB degradation process. The increase in the corresponding k2 values with Bi₂O₃ incorporation and irradiation dose suggests enhanced interactions between MB molecules and the nanocomposite. Nevertheless, the slightly higher R2 values obtained for the pseudo-first-order model indicate that photocatalytic degradation is the predominant kinetic pathway, while adsorption likely plays a complementary role. Overall, the kinetic results demonstrate that EB irradiation effectively enhances the photocatalytic performance of LDPE/PVB/Bi2O3 nanocomposites at 100 kGy,

Table 2 Kinetic parameters using pseudo-first-order and pseudo-second-order models.